Portland ordinary cement: 24-28%

High alumina cement: 5-7%

Anhydrite Cremortive AH48: 5-7%

CaCO3 powder(0.04-0.05mm): Balance

Sand(0.05-0.2mm): 40-45%

PCE Cremortive 5910: 0.1-0.2%

HPMC cocelose 05: 0.08-0.12%

Li2CO3 Cremortive LC99: 0.02-0.06%

Tartaric acid Cremortive TA 03: 0.05-0.1%

Sodium gluconate Cremortive SG 01: 0.05-0.1%

Defoamer Cremortive DF 715P: 0.1-0.2%

RDP ACMEVA 815: 1-2%

Total amount: 100%